Designation

Grade
WC6
UNS
J12072
Standard
ASTM A217/A217M
Density
≈ 7.85 g/cm³
Usual delivery condition
Normalised and tempered

Chemical composition

ElementMass fraction, %
C0.05–0.20
Mn0.50–0.80
Si≤ 0.60
Cr1.00–1.50
Mo0.45–0.65
Febal.

Main elements only. Phosphorus, sulphur and residual-element limits are specified in the standard and are not reproduced here.

Mechanical properties

ConditionTensile strength Rm, min. (MPa)Yield strength Rp0.2, min. (MPa)Elongation, min. (%)
Normalised and tempered485–65527520

Minimum values (or ranges) for separately cast test bars as specified in ASTM A217/A217M.

Characteristics

Corrosion and oxidation behaviour
Not corrosion resistant; coating or other protection required in corrosive environments
Weldability
Possible with qualified procedure; preheat and/or post-weld heat treatment as specified
Machinability
Good in the appropriate heat-treatment condition
Typical applications
Valves Energy High-temperature service Pressure parts

International cross-reference

SystemDesignationRelationship
EN1.7357 (G17CrMo5-5), EN 10213Comparable properties
JISSCPH21 (G 5151)Comparable properties

Casting and processing considerations

Good castability and moderate pouring temperatures. Surface decarburisation from the reaction between metal, shell and atmosphere has to be considered on heat-treated and wear surfaces; machining allowance or a controlled furnace atmosphere are common countermeasures. Section-size sensitivity of quenched and tempered grades should be reflected in the drawing requirements.